请问AR膜怎么做:请问AR膜400NM~700NM R〈0。4%怎么做?6层可以吗?
好象6层优化的效果不好,不过这还要看你所用的膜料了!你膜料的折射率和镀膜件的折射率分别为多少?
我看四层就可以了!!你是指在400-700的平均透过率吧<img src="data/attachment/forum/dvbbs/2004-5/2004516174031731.jpg" border="0" onload="if(this.width>screen.width*0.7) {this.resized=true; this.width=screen.width*0.7; this.alt=\'Click here to open new window\nCTRL+Mouse wheel to zoom in/out\';}" onmouseover="if(this.width>screen.width*0.7) {this.resized=true; this.width=screen.width*0.7; this.style.cursor=\'hand\'; this.alt=\'Click here to open new window\nCTRL+Mouse wheel to zoom in/out\';}" onclick="if(!this.resized) {return true;} else {window.open(\'data/attachment/forum/dvbbs/2004-5/2004516174031731.jpg\');}" onmousewheel="return imgzoom(this);" alt="" />
<

>这是一个6层的。看看可以吗??</P>
<

><img src="data/attachment/forum/dvbbs/2004-5/200451623161423.gif" border="0" onload="if(this.width>screen.width*0.7) {this.resized=true; this.width=screen.width*0.7; this.alt=\'Click here to open new window\nCTRL+Mouse wheel to zoom in/out\';}" onmouseover="if(this.width>screen.width*0.7) {this.resized=true; this.width=screen.width*0.7; this.style.cursor=\'hand\'; this.alt=\'Click here to open new window\nCTRL+Mouse wheel to zoom in/out\';}" onclick="if(!this.resized) {return true;} else {window.open(\'data/attachment/forum/dvbbs/2004-5/200451623161423.gif\');}" onmousewheel="return imgzoom(this);" alt="" />
</P>
光R做的好有啥用,说不定的吸收挺大,真不知谁设计的系统,要这种膜,干脆设计从紫外线到红外全波段AR的膜的了,通用啊。
<TABLE cellPadding=4 cellSpacing=0 width="100%"><TR><TD glow(color=#cccccc,strength=2)" vAlign=center width=*><FONT color=#0000ff><B>yin99</B></FONT> </TD><TD vAlign=center width=25><img src="http://bbs.oecr.com/Skins/Default/ofMale.gif"> </TD><TD vAlign=center width=16></TD></TR></TABLE><

> <img src="http://bbs.oecr.com/images/userface/image1.gif">
<img src="http://bbs.oecr.com/Skins/Default/star/level17.gif">
老兄,光设计出来可以,但实际镀出来可能就不是这么一回事了</P><

>这要跟人家的机台及工艺结合在一起才行</P>
<TABLE cellPadding=4 cellSpacing=0 width="100%"><TR><TD glow(color=#9898BA,strength=2)" vAlign=center width=*><

>同意 <FONT color=#000066><B>mzxnhgs</B></FONT></P><

>理论和实际相差甚远! </P></TD></TR></TABLE>
<

>理論上設計ㄉ出來…一點也不難…</P>
<

>實際上要鍍ㄉ一模一樣…就有些困難…</P>
<

>不過又要鍍ㄉ好,又不脫膜…就需要離子鍍了…而不是傳統ㄉar設計方法了…</P>
<DIV class=quote><B>以下是引用<I>mzxnhgs</I>在2004-5-17 11:37:30的发言:</B>
<TABLE cellSpacing=0 cellPadding=4 width="100%">
<TR>
<TD vAlign=center width=* glow(color='#cccccc,strength=2)"'><FONT color=#0000ff><B>yin99</B></FONT> </TD>
<TD vAlign=center width=25><IMG src="http://bbs.oecr.com/Skins/Default/ofMale.gif"> </TD>
<TD vAlign=center width=16></TD></TR></TABLE>
<

> <IMG src="http://bbs.oecr.com/images/userface/image1.gif">
<IMG src="http://bbs.oecr.com/Skins/Default/star/level17.gif">
老兄,光设计出来可以,但实际镀出来可能就不是这么一回事了</P>
<

>这要跟人家的机台及工艺结合在一起才行</P></DIV>
<

>这个AR膜做起来并不很难,用进口的设备比较容易做。我用国产的电子枪加进口的光控,做过400-1100的AR膜,平均透过率0.6%,基本上能跟设计的相吻合!</P>
<

>传错了</P>
<

>
</P>
<

>yin99:</P><

>这个AR膜做起来并不很难,用进口的设备比较容易做。我用国产的电子枪加进口的光控,做过400-1100的AR膜,平均透过率0.6%,基本上能跟设计的相吻合!</P><

>不知老兄你用的是什么药材?</P>
<

><b><FONT color=#000066>mzxnhgs:</FONT></b></P><

>Nb2O5的折射率为多少?</P><

>你是用什么药料??</P><

>我是用比较普通的tio2和sio2,mgf2啊!!</P>
nb2o5:500nm 2.358<

> 550nm 2.328</P>
我用15层就OK了HTRHDFJFJD FHVFCH NFKGY,ONKDHSRYTCXSEVYRTD UBDRTYCDRYVDRYUMTIFBVUYE
很好镀呀!基材的折射率是多少?
用南光机也很好达到,关键是机器状态要把握的很准确,咱们搞镀膜的,机器有时就象自己的孩子,有时又象老婆.
现在用国产南光或北仪的机器加上我们公司的光控,可以轻松做到400-900 R《1%,400-700 R〈0。3%,国内已有很多公司可以通过它做,需要详细资料可留言,我把资料发给大家看,有需要可以联系13693572892,010-58051723,XLLI@goldway.com.cn
楼上的给我发一份资料,X_X_X_F@SINA.COM
谢谢!
我们的设备可以测量膜料镀制过程中的折射率,可是实时监控镀膜过程中的镀膜曲线的变化,更好更直观的服务于镀膜,提高重复性和生产效率!有问题我们大家可以讨论,E-MAIL:xlli@goldway.com.cn TEL:010-58051723 13693572892,欢迎讨论
K,高档啊,是不是LB机啊??????????????
Nb2o5不用离子源镀,折射率有点低。用Tio2镀的AR膜对透过率有点影响。
引“光R做的好有啥用,说不定的吸收挺大”
请问如何测量吸收,如SiO2,Si3N4,SiNx,a-Si等膜料。
Nb2O5的折射率 550nm处大约2.3。这种材料在使用过程容易翻滚 。
翻滚????何来???????????????????????????????????
用TiO2充氧控制得不好的话,短波处有吸收啊!用ZrO2吧,便宜,不过要注意厚度随折射率变化吖